Sheng Iron currently uses amorphous refractory materials to replace shaped products in heating furnaces. The LN, JR and DGG series products have been the first choice by design institutes and customers for working lining of heating furnaces. DDG series are for water-cooling pipes lining. Characterized by good thermal shock resistance and spalling resistance, they have been applied in more than a hundred heating furnaces domestically,and well received by customers.
Properties specification of LC and ULC
castables for heating furnaceworking lining
Type |
SR-LN-45 |
SR-JRG-1 |
SR-JR-60 |
SR-JR-65 |
SR-JR-70 |
SR-DGG-1 |
SR-DGG-2 |
SR-KZ |
|
Chemical analysis(%) ≥ |
Al2O3 |
45 |
55 |
60 |
65 |
70 |
65 |
65 |
60 |
Bulk density (g/cm3) ≥ |
110℃×24h |
2.20 |
2.30 |
2.30 |
2.40 |
2.50 |
2.45 |
2.40 |
2.70 |
1350℃×3h |
2.20
(1300℃) |
2.25 |
2.20 |
2.30 |
2.40 |
2.40 |
2.30 |
2.60 |
|
Modulus of rupture Mpa ≥ |
110℃×24h |
3 |
3 |
4 |
4 |
5 |
6 |
5 |
4 |
1350℃×3h |
4
(1300℃) |
4 |
5 |
5 |
6 |
8 |
6 |
5 |
|
Compressive strength Mpa≥ |
110℃×24h |
30 |
30 |
35 |
30 |
30 |
40 |
35 |
30 |
1350℃×3h |
40
(1300℃) |
45 |
50 |
50 |
50 |
55 |
50 |
50 |
|
Permanent change (%) |
1350℃×3h |
±0.5
(1300℃) |
±0.5 |
±0.5 |
±0.5 |
±0.5 |
±0.5 |
±0.5 |
0~+1.0 |
Service temperature (℃) |
1300 |
1400 |
1400 |
1500 |
1550 |
1550 |
1500 |
1400 |
Please fill in the information you want to know in the form below, and we will contact you as soon as possible: